ELANTAS RN-1501

Harmonization Code : 3910.00.00.90 | Silicones in Primary Forms; Others

ELANTAS RN-1501

Main features

  • Heat-Reduced Resin Viscosity
  • Three-Minute Meter-Mix Window
  • High-Elongation Cast Elastomer

Product Description

CONATHANE RN-1501 Liquid Urethane Prepolymer is a PTMEG polyether liquid urethane prepolymer for producing flexible cast elastomers. Typical viscosity decreases from 17,000 cP at 25 deg C to 500 cP at 100 deg C, providing a defined temperature-dependent processing profile. With CONACURE AH-40 at 100/12.5 parts by weight, the system has a 3-minute work life and forms a Shore A 90 elastomer with 7,500 psi tensile strength and 520% elongation. Applications include industrial truck tires, rolls, gears, die pads, and abrasion-resistant belts.

Key features

  • Temperature-Dependent Viscosity: Typical viscosity decreases from 17,000 cP at 25 deg C to 500 cP at 100 deg C.
  • Three-Minute Work Life: The RN-1501 and CONACURE AH-40 configuration has a 3-minute mixed work life.
  • High-Elongation Elastomer: The specified curative system reaches 520% elongation with Shore A 90 hardness.

Applications / Suitable for

  • Industrial truck tires
  • Rolls, gears, and die pads
  • Abrasion-resistant belts
Product Family

ELANTAS RN-1501

Catalog Product

Unlike other products we offer, the products listed on this page cannot currently be ordered directly from the website.

TDS, SDS & Technical Documents

Technical Specifications

General Properties
Color Color
Clear light amber
Specific Gravity Specific Gravity
1.06

Additional Information

Technical properties

As-supplied / before-processing properties

Typical resin and process data for RN-1501 with the specified CONACURE AH-40 configuration.

Property Value Unit Method / condition
NCO content 4.10 to 4.40 % Typical RN-1501 resin
Specific gravity 1.06 - RN-1501 at 25 deg C
Viscosity 17,000 cP RN-1501 at 25 deg C
Viscosity 500 cP RN-1501 at 100 deg C
Mix ratio 100/12.5 parts by weight RN-1501 / CONACURE AH-40
Work life 3 minutes RN-1501 with CONACURE AH-40
Demold time 45 minutes Mold at 60 deg C; RN-1501 with CONACURE AH-40
Cure and post-cure 4 + 16 hours Cure 4 hours at 100 deg C; post-cure 16 hours at 100 deg C
Technical properties

After-processing / final-state properties

Typical cured-elastomer properties for RN-1501 combined with CONACURE AH-40 at 100/12.5 parts by weight.

Property Value Unit Method / condition
Hardness 90 Shore A RN-1501 / CONACURE AH-40
Tensile strength 7,500 psi RN-1501 / CONACURE AH-40
100% modulus 1,050 psi RN-1501 / CONACURE AH-40
300% modulus 1,650 psi RN-1501 / CONACURE AH-40
Tear strength 400 pli Die C; RN-1501 / CONACURE AH-40
Elongation 520 % RN-1501 / CONACURE AH-40
Specific gravity 1.10 - Cured elastomer at 25 deg C